| Steel | Thermal Expansion* (μm/mK) | Thermal Conductivity* (W/mK) | Specific Heat Capacity (J/kgK) |
|---|---|---|---|
| SA210 P265GH (EN 1.0425) | 14.0 | 46 | 470 |
| SS 304 (EN 1.4306) | 17.7 | 19.0 | 480 |
| SS 309 (EN 1.4828) | 17.5 | 18.7 | 480 |
| 16Mo3 (EN 1.5415) | 13.5 | 43.1 | 470 |
| 10CrMo9-10 (EN 1.7380) | 13.5 | 37.8 | 470 |
| 7CrWVMoNb9-6 (EN 1.8201) | 470 | ||
| Inconel 625 | 13.5 | 14.1 | 440 |
| Incoloy 825 | 15.6 | 15.4 | 440 |
| Sanicro 28 | 16.0 | 17 | 480 - 555 |
| Sanicro 38 | 15.1 | 16 | |
| Sanicro 67 | 14.9 | 16 |